钛基钎焊粉使用活性钎料钎焊的最低温度为 850 °C,随着温度的增高可以改善钎料的润湿性。该钎料的钎焊需要氩气保护或者真空度低于(10-3 Pa),为了防止银蒸发,钎焊温度为900 °C-1000 °C
Ti-flo™ Brazing Filler Metals for Titanium Alloys
Alloy | Ti | Zr | Ni | Cu | Ag | Al | Other | Melting Range °C |
Ag-Al | 95 | 5 | 780-830 | |||||
Ti-950 | 70 | 15 | 15 | 0.3% max. | 902-950 | |||
Ti-1 | 54 | 27.5 | 18.5 | 927-946 | ||||
Ti-2 | 60 | 25 | 15 | 901-915 | ||||
Ti-3 | 25 | 25 | 50 | 780-815 | ||||
Ti-4 | 40 | 20 | 20 | 20 | 848-856 | |||
Ti-5 | 44 | 24 | 16 | 16 | Mo 0.5 | 835-850 | ||
Ti-6 | 37.5 | 37.5 | 10 | 15 | 805-815 | |||
Ti-7 | 35 | 35 | 15 | 15 | 770-820 |
Other filler metals for Brazing of Titanium Alloys
Alloy | Pd | Ag | Cu | Ti | Other | Melting Range °C |
Ag-82 | 9 | 82 | 9 Ga | 845-880 | ||
Ag-92.5 | 92.5 | 7.5 | 805-890 | |||
Ag | 99.99 | 960 | ||||
AgCuTi-1 | 92.75 | 6 | 1.25 | 800-900 | ||
AgCuTi-2 | 68.8 | 26.7 | 4.5 | 830-850 | ||
AgCuTi-3 | 64 | 34.2 | 1.8 | 780-810 | ||
AgCuTi-4 | 70.5 | 26.5 | 3.0 | 780-805 | ||
Ag-96 | 96 | 4 | 1000-1050 | |||
AgCuIn | 98.4 | 0.6 | In 1 | 948-959 |